Polymer Properties |
Min.
|
Max.
|
Method
|
|
|
Mooney Viscosity ML1+4100℃ |
41 |
49
|
GB/T 1232.1
|
|
|
Volatile Matter % |
---
|
0.50
|
ISO 248
|
|
|
Ash % |
---
|
0.20
|
GB/T 4498
|
|
|
Compound Properties/T 8660-2008; Cure at 145℃
|
||||
|
Compound, ML1+4100℃ |
---
|
65
|
GB/T 1232.1
|
|
|
Tensile Strength MPa,35min |
13.2
|
---
|
GB/T 8660-2008
|
|
|
Elongation % 35min |
330
|
---
|
GB/T 8660-2008
|
|
|
Modulus MPa
|
25min |
7.0 |
12.0 |
GB/T 8660-2008 |
|
35min |
8.0 |
13.0 |
GB/T 8660-2008 |
|
|
50min |
8.0 |
13.0 |
GB/T 8660-2008 |
|
BR9104(Neodymium catalyst) Specification:
|
Polymer Properties |
Min.
|
Max.
|
Method
|
|
Mooney Viscosity ML(1+4)100℃ |
38 |
48
|
GB/T 1232.1
|
|
Volatile Matter % |
---
|
0.50
|
GB/T24131.1
|
|
Ash % |
---
|
0.30 |
GB/T4498.1
|
|
Compound Mooney Viscosity ML(1+4)100℃
|
---
|
80
|
GB/T 1232.1
|
|
Modulus, MPa
|
8.5
|
13.5 |
GB/T 8660 C2
|
|
Tensile Strength, MPa
|
15.0 |
---
|
GB/T 8660 C2
|
|
Elongation,%
|
360 |
--
|
GB/T 8660 C2
|
|
Recipe: GB/T 8660; Curve condition: 145℃*35min
|
|||
Packing of Polybutadiene Rubber
PE film and kraft paper bag packing for piece of rubber or MB5, net weight: 25.0±0.25kg/bag
PE film and Kraft paper bag packing for piece of rubber or MB5(GPS5), net weight: 25.0±0.25kg/bag.
For polybutadiene rubber price or more information, please feel free to contact us!
If you need any kinds of butyl rubber, please contact us, as a professional rubber raw materials company, YuSheng is willing to offer you high quality products.
Good deal: buying from seller
|
This page is about importers and exporters of Polybutadiene Rubber Search in a category : B2B Services Search in a category : polybutadiene, rubber |
Thursday, June 16, 2016
Application Method 1. Glue is applied on textile or leather. 2. Patterned or fully coated glue is fixed by heat before foil transfer properly. 3. Stamping the foil ,heat: 130C-150C, pressure 4-6 bar, touch time 3-5 s. 4. Discard the carrier film after stamping process.Different...
Tuesday, April 28, 2026
Quantity : 4 - Price : 14,90 €
Size in the pack From S TO XXL Compositions 70% ACRYLIC, 30% WOOL Chic styles ANTHRACITE color in the pack COL properties BALL LEARN MORE Cowl neck sweater has buttons and links resserages. This all twisted pull on the chest consists of a small leather shield down the size...
Friday, April 05, 2013
Quantity : 250 comman - Price : 0,60 €
Anti-glare (matte), hard-coated, dirt-repellent, easy to install and can be removed without leaving any traces The screen protector is designed for application on electronic screens and offers reliable protection against scratches and dirt. The film surface is dull and to mitigate...